Defocus is set with the focus tube (also called the gas tube) on the welding torch, and it is about getting the laser light to where it needs to be. This video shows where to start on steel with the THEO MA1 Series, why the material’s reflectivity matters more than its thickness, and what a wrong setting does to the weld and to your protective window.

Start at minus two

For wire-assist welding on steels, including carbon steel, stainless steel and galvanized steel, set the defocus to minus two by default. Minus two is the number to remember on your MA1.

Reflectivity matters more than thickness

Alloys reflect laser light differently, and that changes the right setting more than the material’s thickness does. In the video, thick stainless steel plate welds with wire at minus two on the THEO MA1 ULTRA. A 1 mm to 3 mm aluminum T-joint needed a different defocus setting before the wire weld showed any penetration.

At the right setting, the aluminum bead with wire was a little crowned but had good penetration. Pulled out to zero, the top still looked fine, but the wobble showed like a broken zipper on the sides and there was barely any penetration.

Fusion welding on aluminum

For autogenous fusion only on aluminum, the video rolls the edge of a 2 mm 5052 outside corner at minus two. Fusion still needs negative defocus, but not as much, because no reflective filler wire is melted into the reflective base material. On outside corners, the video still uses a wire-assist welding nozzle, without wire, to balance the torch on the corner.

What a wrong setting does

The video shows on thin aluminum what happens when only the defocus changes, with every machine setting left as it was:

  • Focus tube pushed all the way back: the defocus is about 13 mm further out than it should be. For the operator everything looks the same and the guide beam still lines up, but the result is a braze, not a weld.
  • Plus 15: part of the light reflects back up into the tool.
  • Minus five, only three steps further than the default: the bead comes out flat, more than needed.

Across the wrong attempts you can see wormholes in the welds, and every one of them burns aluminum specks into the protective window. It will not kill your machine, but it slows you down. So keep an eye on the defocus, and check that nobody has pushed the focus tube back.